CONATHANE EN-5317 Polyurethane Encapsulant
Harmonization Code : 3909.20.00.90 | Amino-resins, phenolic resins and polyurethanes, in primary forms : Melamine resins : Other
Main features
- 300 cP Mixed Viscosity
- 1:1 Controlled Mixing
- Clear Polyurethane for Potting and Bonding
Product Description
CONATHANE EN-5317 is an unfilled, two-component polyurethane system for potting, encapsulating, and bonding electrical and electronic assemblies. Part A urethane prepolymer and DP32127 Part B curative mix at 100:97 by weight or 1:1 by volume. The mixed system has a typical initial viscosity of 300 cP and a 10-15 minute work life at 25 C. Documented applications include electrical potting, electronic encapsulation, and adhesive bonding. Use either 7-10 days at 25 C or 16 hours at 80 C.
Key features
- Flow and dispensing: Low initial mixed viscosity of 300 cP at 25 C.
- Mix ratio: Cartridge-friendly 1:1 mix ratio by volume.
- Application fit: Clear polyurethane for potting, encapsulation, and bonding.
Applications
- Electrical potting
- Electronic encapsulation
- Adhesive bonding
TDS, SDS & Technical Documents
Technical Specifications
General Properties
Physical Properties
Mechanical Properties
Additional Information
CONATHANE® EN-5317 DP32127
CONATHANE® EN-5317 DP32127, formerly CONAP EN-5317, is a two-component, unfilled polyurethane potting and encapsulating compound used for electrical and electronic assemblies exposed to challenging environmental conditions involving high ambient temperature, humidity, and exposure to sunlight.
The material is mixed at a 1:1 ratio by volume (Part A to Part B) before application. It supports hand-mix bench processing, cartridge dispensing, meter-mix bench processing, and meter-mix vacuum processing. After application, the material can be cured for 7 to 10 days at 25°C or for 16 hours at 80°C.
CONATHANE® EN-5317 DP32127 has separate safety data sheets for Part A and Part B. The Safety data sheet button above opens the Part A document.
Low-viscosity potting for electronic assemblies
- 1:1 mix ratio by volume: Cartridge-friendly dispensing supports convenient mixing and processing.
- Low viscosity: Initial mixed viscosity of 300 cP helps material flow into assemblies and components.
- UV-stable polyurethane system: Suitable for electronic assemblies exposed to sunlight, humidity, and elevated temperatures.
- Environmental resistance: Documented thermal shock, heat aging, and humidity aging test results support evaluation for challenging conditions.
- Electronic assembly protection: Formulated for electronic circuits, components, and assemblies requiring protection from humidity, temperature exposure, and outdoor environments.
Two-component mixing and curing
Highly recommended for
CONATHANE® EN-5317 DP32127 is formulated for electronic circuits, components, and assemblies requiring protection from humidity, temperature exposure, and outdoor environments.
Typical Properties of Material as Supplied
| Property | CONATHANE® EN-5317 Part A Urethane Prepolymer |
CONATHANE® EN-5317 DP32127 Part B Curative |
Conditions |
|---|---|---|---|
| Viscosity | 1,000 cP | 220 cP | 25°C / 77°F |
| Specific Gravity | 1.06 | 1.03 | 25°C / 77°F |
| Appearance | Clear | Clear | — |
| Mix Ratio — Parts by Weight | 100 | 97 | Parts by weight |
| Mix Ratio — Parts by Volume | 100 | 100 | Parts by volume |
| Flashpoint | > 94°C > 201°F |
> 94°C > 201°F |
ASTM D93 |
Mix ratios refer to Part A and Part B respectively. The ratio by weight differs from the ratio by volume.
Typical Properties of Mixed Materials
| Property | Value | Conditions |
|---|---|---|
| Mixed Viscosity (Initial) | 300 cP | 25°C / 77°F |
| Work Life | 10–15 mins | 25°C / 77°F |
| Tack Free (Thin Film) | 10 mins | 80°C / 176°F |
Typical Physical Properties
Specimens cured for 16 hours at 80°C / 176°F.
| Property | Value | Test Method | Condition |
|---|---|---|---|
| Shore Hardness | A 70 | ASTM D2240 | 25°C / 77°F |
| Tensile Strength | 2,200 psi | ASTM D412 | 25°C / 77°F |
| Ultimate Elongation | 200% | ASTM D412 | 25°C / 77°F |
| Tear Strength | 110 pli | ASTM D624 | 25°C / 77°F |
| Linear Shrinkage | < 0.1% | MIL-M-24041C | — |
Lap Shear Properties
| Substrate | Primer Condition | Lap Shear Value |
|---|---|---|
| Steel | Without primer | 775 psi |
| Steel | Primed with CONAP® AD-1146 | 790 psi |
| Aluminum | Without primer | 310 psi |
| Aluminum | Primed with CONAP® AD-1146 | 670 psi |
Mechanical Aging Tests
CONATHANE® EN-5317 DP32127 passed 10 cycles of thermal shock testing from -70°C to 130°C under MIL-I-16923E. Separate heat aging and humidity aging tests recorded tack-free hardness results after 1,000 hours of exposure under the stated conditions.
| Property | Value / Observation | Test Method | Condition |
|---|---|---|---|
| Thermal Shock | Pass 10 cycles | MIL-I-16923E | -70°C to 130°C |
| Heat Aging | Shore A 87 Clear, no tack |
— | 1,000 hours at 70°C / 158°F |
| Humidity Aging | Shore A 67 Slightly yellow, no tack |
— | 1,000 hours at 85°C / 85% RH |
The values above describe the stated aging test results and conditions. The thermal shock test range is not presented as a continuous operating-temperature rating.
Application Methods
CONATHANE® EN-5317 DP32127 supports the following potting and casting methods.
Potting / Casting
Potting / Casting
Potting / Casting
Potting / Casting
Application and Curing Schedule
- Measure EN-5317 Part A and EN-5317 DP32127 Part B according to the specified mix ratio.
- Pour both components into a clean metal or glass container.
- Mix thoroughly using a metal or glass stirrer until a uniform blend is achieved.
- Ensure the container is large enough to accommodate any frothing during degassing.
- Degas the mixture at room temperature under a vacuum greater than 27 in. Hg until entrapped air is removed.
Use one of the following curing schedules:
- 7–10 days at 25°C / 77°F, or
- 16 hours at 80°C / 176°F.
Start the cure time only after the material reaches the specified cure temperature. Adjust cure conditions as needed to achieve the desired performance for the application.
Shelf Life, Transportation & Storage
Store at 20–30°C / 68–86°F in a dry, controlled environment out of direct sunlight.
This material should be suitable for use when stored under these conditions in its original sealed containers for twelve (12) months from the date of shipment. Cartridge packaging may adjust product shelf life.
Failure to store the product as recommended may lead to deterioration in product performance.
The product is sensitive to moisture and atmospheric humidity. Containers, once opened, should be used immediately or blanketed with dry air or nitrogen before resealing.
Refer to the separate safety data sheets for Part A and Part B when reviewing handling and safety information.
CONATHANE® EN-5317 Part A may crystallize upon storage or during shipment. If crystallization has occurred, heat to 60°C, mix thoroughly, and cool to room temperature before processing.
Used for Agricultural Controllers
Agricultural controllers are used for modern farming systems such as irrigation control, autonomous equipment, and crop monitoring devices. These electronic assemblies are constantly exposed to moisture, dust, contaminants, temperature changes, and other harsh environmental conditions that can affect reliability.
CONATHANE® EN-5317 DP32127 can be used for potting and encapsulation of electrical and electronic assemblies of these agricultural controllers, providing protective layers around sensitive components. This helps reduce exposure to environmental conditions and supports reliable operation in demanding agricultural environments.

Used for Automotive Electronics
Automotive electronics and sensors are exposed to challenging environmental conditions, including moisture, dust, chemicals, vibration, and high ambient temperature. Electronic components continue to increase in both electric and conventional vehicles, making protection of these assemblies important for maintaining reliability, performance, and a long service life.
CONATHANE® EN-5317 DP32127 can be used for potting and encapsulation of electrical and electronic assemblies of electronic control modules, sensors, and circuit boards found in automotive applications. The material helps shield sensitive components from environmental exposure and mechanical stress, supporting the durability and reliability of automotive electronic systems.

Used for LED Lighting

LED signage, controllers, and drivers must provide consistent performance while operating in environments that are exposed to moisture, temperature fluctuations, and prolonged outdoor exposure. Protecting electronic assemblies is critical to maintaining brightness, reliability, and long-term system performance.
CONATHANE® EN-5317 DP32127 can be used for potting and encapsulation of electrical and electronic components within LED signage and controller systems. This creates a protective barrier around sensitive circuitry, helping reduce environmental exposure and supporting reliable operation in LED lighting applications.
Used for Smart Meters

Smart electricity, water, and gas meters rely on electronic assemblies that must operate reliably under varying environmental conditions. Moisture exposure and temperature fluctuations can affect sensitive components, potentially compromising meter performance and measurement accuracy.
CONATHANE® EN-5317 DP32127 can be used to encapsulate printed circuit boards and electronic components within smart meters, including inductors, coils, and voltage regulators. By forming a protective barrier around these assemblies, the material helps reduce exposure to environmental conditions that could affect their long-term reliability.